5xxx Series · Temper H22 / H111 · EN 485 / EN AW-5754

5754 Aluminum — Properties, Weight Calculator & Engineering Datasheet

European automotive body, tread plate, and marine sheet. ~3% Mg content makes it immune to elevated-temperature sensitization unlike 5083.

Specific Strength (Rp0.2 / ρ)
48.7 kN·m/kg
True ρ = 2.67 g/cm³

Density (ρ)

2.67 g/cm³

2670 kg/m³ · 0.0965 lb/in³

Yield (Rp0.2)

130 MPa

19 ksi (0.2% offset)

Tensile (Rm)

220 MPa

32 ksi ultimate

Shear Strength (τu)

140 MPa

Ultimate shear

Fatigue Limit

100 MPa

5×10⁸ cycles RR Moore

Bearing Yield

250 MPa

e/D = 2.0 pin/rivet

Elongation (A)

17%

Min bend R ≈ 1.5×t

Modulus (E)

70 GPa

Shear G ≈ 27 GPa

Hardness

55 HB

Temper H22 / H111

α Thermal Exp.

23.7×10⁻⁶/K

20–100 °C linear

k Thermal Cond.

132 W/m·K

600 – 645 °C

Elec. Cond.

34% IACS

CNC Vc ≈ 300 m/min

Interactive Engineering Workbench · 5754 Aluminum (EN 485 / EN AW-5754)

5754 Aluminum Live Calculator & Design Verification Suite

True Mass (2.67 g/cm³)
8.01 kg
17.66 lb (8.010 kg/pc)
If Assumed ρ = 2.70 g/cm³
8.10 kg
Δ = -0.09 kg (-1.11%)
Estimated Material Cost
$54.47
Vol: 3000 cm³ · A: 3000 mm²
Engineering Mass Traceability Note

5754 Aluminum contains alloying elements (5xxx series) that shift its density to 2.67 g/cm³ (2670 kg/m³). On a 1-piece batch, generic 2.70 g/cm³ calculators miscalculate shipping and structural mass by 90 grams.

Chemical Composition Limits (wt% per EN 485 / EN AW-5754)

Nominal elemental mass fractions governing density (2.67 g/cm³), precipitation hardening, and weldability.

EN 573-3 / AA Registered Limits
Al
94.2–97.4%
Cu
≤ 0.10%
Mg
2.6–3.6%
Mn
≤ 0.50%
Si
≤ 0.40%
Zn
≤ 0.20%
Cr
≤ 0.30%
Fe
≤ 0.40%

Standard Nominal Density vs Generic 2.70 g/cm³ Baseline

Nominal standard density for 5754 Aluminum is 2.67 g/cm³ (2670 kg/m³ per EN 485 / EN AW-5754). Assuming a generic 2.70 g/cm³ aluminum density introduces a -1.11% mass discrepancy across BOM, structural payload, and freight logistics calculations.

Normative Specification vs Lot Inspection: Values shown are normative nominal design baselines per EN 485 / EN AW-5754 and EN 573-3. Lot-specific physical properties and chemical compositions are documented on manufacturer Mill Test Certificates (EN 10204 Type 3.1 / 3.2). Mechanical strength values represent standard minimum guarantees for extruded profiles (typically wall thickness t ≤ 5 mm); thicker gauges, plate products (EN 485), and specific tempers follow dedicated standard sub-clauses.

1 m² × 10 mm plate (True ρ = 2.67)

26.70 kg

Same plate if assumed ρ = 2.70

27.00 kg

Mass Discrepancy per Plate

-0.30 kg (-0.66 lb)

Weldability (EN 1999 / AWS)

Excellent

TIG/MIG weldable using ER4043 or ER5356 filler wire.

CNC Machinability

Fair

Recommended 3-flute carbide Vc ≈ 300 m/min.

Corrosion & Anodizing

Excellent

Melting range: 600 – 645 °C.

Typical Industrial Applications

  • • Automotive inner body panels
  • • 5-bar checker tread plate
  • • Pressure vessels & silos
  • • Welded chemical tanks

Engineering Pitfalls & Design Warnings

  • ⚠ Check temper carefully — H111 yield (80 MPa) vs H22 yield (130 MPa) differs substantially
  • ⚠ Not a substitute for 6082-T6 structural extrusions

Compare 5754 Aluminum & Explore All Aluminum Alloys

Methodology Tier 1 Normative Reference: EN 485 / EN AW-5754 / EN 573-3 / EN 485-2 / MMPDS. Values are typical handbook figures for temper H22 / H111.