3xxx Series · Temper H14 · ASTM B209 / EN AW-3003

3003 Aluminum — Properties, Weight Calculator & Engineering Datasheet

General-purpose Al-Mn sheet alloy. 20% stronger than 1100 with excellent formability and atmospheric corrosion resistance.

Specific Strength (Rp0.2 / ρ)
53.1 kN·m/kg
True ρ = 2.73 g/cm³

Density (ρ)

2.73 g/cm³

2730 kg/m³ · 0.0986 lb/in³

Yield (Rp0.2)

145 MPa

21 ksi (0.2% offset)

Tensile (Rm)

180 MPa

26 ksi ultimate

Shear Strength (τu)

110 MPa

Ultimate shear

Fatigue Limit

62 MPa

5×10⁸ cycles RR Moore

Bearing Yield

210 MPa

e/D = 2.0 pin/rivet

Elongation (A)

8%

Min bend R ≈ 1×t

Modulus (E)

69 GPa

Shear G ≈ 27 GPa

Hardness

40 HB

Temper H14

α Thermal Exp.

23.2×10⁻⁶/K

20–100 °C linear

k Thermal Cond.

193 W/m·K

643 – 654 °C

Elec. Cond.

46% IACS

CNC Vc ≈ 260 m/min

Interactive Engineering Workbench · 3003 Aluminum (ASTM B209 / EN AW-3003)

3003 Aluminum Live Calculator & Design Verification Suite

True Mass (2.73 g/cm³)
8.19 kg
18.06 lb (8.190 kg/pc)
If Assumed ρ = 2.70 g/cm³
8.10 kg
Δ = +0.09 kg (+1.11%)
Estimated Material Cost
$55.69
Vol: 3000 cm³ · A: 3000 mm²
Engineering Mass Traceability Note

3003 Aluminum contains alloying elements (3xxx series) that shift its density to 2.73 g/cm³ (2730 kg/m³). On a 1-piece batch, generic 2.70 g/cm³ calculators miscalculate shipping and structural mass by 90 grams.

Chemical Composition Limits (wt% per ASTM B209 / EN AW-3003)

Nominal elemental mass fractions governing density (2.73 g/cm³), precipitation hardening, and weldability.

EN 573-3 / AA Registered Limits
Al
96.7–99.0%
Cu
0.05–0.20%
Mg
—
Mn
1.0–1.5%
Si
≤ 0.60%
Zn
≤ 0.10%
Cr
—
Fe
≤ 0.70%

Standard Nominal Density vs Generic 2.70 g/cm³ Baseline

Nominal standard density for 3003 Aluminum is 2.73 g/cm³ (2730 kg/m³ per ASTM B209 / EN AW-3003). Assuming a generic 2.70 g/cm³ aluminum density introduces a +1.11% mass discrepancy across BOM, structural payload, and freight logistics calculations.

Normative Specification vs Lot Inspection: Values shown are normative nominal design baselines per ASTM B209 / EN AW-3003 and EN 573-3. Lot-specific physical properties and chemical compositions are documented on manufacturer Mill Test Certificates (EN 10204 Type 3.1 / 3.2). Mechanical strength values represent standard minimum guarantees for extruded profiles (typically wall thickness t ≤ 5 mm); thicker gauges, plate products (EN 485), and specific tempers follow dedicated standard sub-clauses.

1 m² × 10 mm plate (True ρ = 2.73)

27.30 kg

Same plate if assumed ρ = 2.70

27.00 kg

Mass Discrepancy per Plate

+0.30 kg (0.66 lb)

Weldability (EN 1999 / AWS)

Excellent

TIG/MIG weldable using ER4043 or ER5356 filler wire.

CNC Machinability

Fair

Recommended 3-flute carbide Vc ≈ 260 m/min.

Corrosion & Anodizing

Excellent

Melting range: 643 – 654 °C.

Typical Industrial Applications

  • • HVAC ductwork & roofing
  • • Brazed heat exchangers
  • • Storage tanks & pressure vessels
  • • Architectural sheet & signage

Engineering Pitfalls & Design Warnings

  • ⚠ Not a load-bearing structural frame alloy
  • ⚠ H14 work-hardened temper locally anneals in the weld HAZ

Compare 3003 Aluminum & Explore All Aluminum Alloys

Methodology Tier 1 Normative Reference: ASTM B209 / EN AW-3003 / EN 573-3 / EN 485-2 / MMPDS. Values are typical handbook figures for temper H14.